Grade 35CrMo
Corresponding Standard JB /T 6396-2006
Specification for The Heavy Alloy Structural Steel Forings
Classification Alloy Steel
35CrMo Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo
Minimum Value 0.32 0.17 0.4 - - 0.8 - - 0.15
Maximum Value 0.4 0.37 0.7 0.035 0.035 1.1 0.3 0.2 0.25
35CrMo Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
≤100 Tempering ≥735 ≥540 ≥15 ≥45 217~269 ≥47
101~300 Tempering ≥685 ≥490 ≥15 ≥45 207~255 ≥39
301~500 Tempering ≥635 ≥440 ≥15 ≥35 196~255 ≥31
501~800 Tempering ≥590 ≥390 ≥12 ≥30 176~241 ≥23

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!