Grade 34CrNi3Mo
Corresponding Standard JB /T 6396-2006
Specification for The Heavy Alloy Structural Steel Forings
Classification Alloy Steel
34CrNi3Mo Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo
Minimum Value 0.3 0.17 0.5 - - 0.7 2.75 - 0.25
Maximum Value 0.4 0.37 0.8 0.035 0.035 1.1 3.25 0.2 0.4
34CrNi3Mo Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
≤100 Tempering ≥900 ≥785 ≥14 ≥40 269~321 ≥54
101~300 Tempering ≥855 ≥735 ≥14 ≥38 255~302 ≥47
301~500 Tempering ≥805 ≥685 ≥13 ≥35 241~286 ≥31