Grade C85S
European Standard Steel Grade 1.1269
Corresponding Standard EN 10132-4-2002
Cold rolled narrow steel strip for heat treatment Ð Technical delivery conditions Ð Part 4: Spring steels and other applications
Classification Spring Steel
C85S Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo
Minimum Value 0.8 0.15 0.4 - - - - -
Maximum Value 0.9 0.35 0.7 0.025 0.025 0.4 0.4 0.1
C85S Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
0.3≤t≤3 Annealing (+A) or Annealing and Flattening (+LC) ≤670 ≤535 ≥15 HV
≤210
0.3≤t≤3 Cold Rolled (+CR) ≤1190 ≤325
0.3≤t≤3 Tempering (+QT) 1200~2000 370~600
Approximate Comparison Table Spring Steel
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France European Standard Russia Sweden United Kingdom
GB ISC CNS JIS KS AISI UNS ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade GOST SS14 BS EN/BS
85 U20852 SUP3 SUP3 SPS1 1086 G10860 Type DC Ck85
C85S
1.1269
1.1269
XC85 C85S 1.1269 85A ≈1774 060A86
CS80
C85S Corresponding Standards(Same grade name, different standards)