Grade PCrNi3MoVA
Corresponding Standard GJB 3783A-2015
Specification for Steel Bars and Steel Forgings for Barrel of Middle-Small Caliber Quick Firing Arms
Classification Alloy Steel
PCrNi3MoVA Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo V
Minimum Value 0.34 0.17 0.25 - - 1.2 3 - 0.35 0.1
Maximum Value 0.41 0.37 0.5 0.02 0.02 1.5 3.25 0.2 0.45 0.25
PCrNi3MoVA Mechanical Properties
condition Mark
Heat Treatment or Condition
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
Steel bars or forgings, transverse sample; t=25 Strength Grade P-635 Normalizing + Quenching + Tempering Specified Proportional Limit σp
635
≥30 ≥20
Steel bars or forgings, transverse sample; t=25 Strength Grade P-685 Normalizing + Quenching + Tempering Specified Proportional Limit σp
685
≥30 ≥20
Steel bars or forgings, transverse sample; t=25 Strength Grade P-735 Normalizing + Quenching + Tempering Specified Proportional Limit σp
735
≥30 ≥17
Steel bars or forgings, transverse sample; t=25 Strength Grade P-785 Normalizing + Quenching + Tempering Specified Proportional Limit σp
785
≥30 ≥17
Steel bars or forgings, transverse sample; t=25 Strength Grade P-835 Normalizing + Quenching + Tempering Specified Proportional Limit σp
835
≥25 ≥17
Steel bars or forgings, transverse sample; t=25 Strength Grade P-885 Normalizing + Quenching + Tempering Specified Proportional Limit σp
885
≥25 ≥15
Steel bars or forgings, transverse sample; t=25 Strength grade P-930 Normalizing + Quenching + Tempering Specified Proportional Limit σp
930
≥25 ≥15
Steel bars or forgings, transverse sample; t=25 Strength grade P-980 Normalizing + Quenching + Tempering Specified Proportional Limit σp
980
≥25 ≥15

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!