Grade G10MnMoV6-3
European Standard Steel Grade 1.5410
Corresponding Standard EN 10340-2007
Steel castings for structural uses
Classification Cast Steel
G10MnMoV6-3 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo V
Minimum Value - - 1.2 - - - - - 0.2 0.05
Maximum Value 0.12 0.6 1.8 0.025 0.02 0.3 0.4 0.3 0.4 0.1
G10MnMoV6-3 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤50 Quenching 1 (+QT1) 500~650 ≥380 ≥22 ≥60 (room temperature); ≥27 (-20°C)
50<t≤100 Quenching 1 (+QT1) 480~630 ≥350 ≥22 Room Temperature
≥60
100<t≤150 Quenching 1 (+QT1) 480~630 ≥330 ≥20 Room Temperature
≥60
150<t≤250 Quenching 1 (+QT1) 450~600 ≥330 ≥18 Room Temperature
≥60
t≤50 Quenching 2 (+QT2) 600~750 ≥500 ≥18 ≥60 (room temperature); ≥27 (-20°C)
50<t≤100 Quenching 2 (+QT2) 550~700 ≥400 ≥18 Room Temperature
≥60
100<t≤150 Quenching 2 (+QT2) 500~650 ≥380 ≥18 Room Temperature
≥60
150<t≤250 Quenching 2 (+QT2) 460~610 ≥350 ≥18 Room Temperature
≥60
t≤100 Quenching + Tempering 3 (+QT3) 520~650 ≥400 ≥22 ≥60 (room temperature); ≥27 (-20°C)