Grade G20Mn5
European Standard Steel Grade 1.6220
Corresponding Standard EN 10340-2007
Steel castings for structural uses
Classification Cast Steel
G20Mn5 Chemical Element Composition Content (%)
Component C Si Mn P S * Cr Ni Cu Mo V More
Minimum Value 0.17 - 1 - - - - - - - Cr+Mo+Ni+V≤1
Maximum Value 0.23 0.6 1.6 0.02 0.02 0.3 0.8 0.3 0.12 0.03
G20Mn5 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤30 Normalizing (+N) 500~650 ≥300 ≥20 ≥50 (room temperature); ≥27 (-30°C)
t≤100 Quenching and Tempering (+QT) 500~650 ≥300 ≥22 ≥60 (room temperature); ≥27 (-40°C)
Approximate Comparison Table Cast Steel
China Germany European Standard
GB DIN EN/DIN EN Numerical Grade
ZG20SiMn GS-20Mn5V G20Mn5 1.6220
G20Mn5 Corresponding Standards(Same grade name, different standards)