Grade ML15MnVB
China ISC A73154
Corresponding Standard GB /T 6478-2015
Steels For Cold Heading And Cold Extruding
Classification Alloy Steel
Properties Forgability
ML15MnVB Chemical Element Composition Content (%)
Component C Si c Mn P S V B b Al a
Minimum Value 0.13 0.1 1.2 - - 0.07 0.0008 0.02
Maximum Value 0.18 0.3 1.6 0.025 0.025 0.12 0.0035 -
ML15MnVB Mechanical Properties
diameter
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
d=25 (Sample diameter) Quenching temperature 860~900°C oil quenching, tempering temperature 340~380°C ≥900 ≥720 ≥10 ≥45 Hot Rolled State
≤207