Grade 38CD 4
Corresponding Standard NF A 35-557-1983
Iron And Steel — Heat Treatable Steels for Externally Threaded, High Performance Fasteners for Engineering Purposes.
Classification Alloy Steel
Properties High Strength
38CD 4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Mo
Minimum Value 0.35 0.1 0.6 - - 0.9 0.15
Maximum Value 0.41 0.4 0.9 0.035 0.035 1.2 0.25
38CD 4 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Bar, coil; d = 40 Oil Quenching - - - HRC42 -
Bar, coil; d = 32 Oil Quenching - - - HRC45 -
Bar, Coil; d=20 Oil Quenching - - - HRC48 -
Bar, Coil; d≤20 Quenching and Tempering 1130~1330 ≥910 ≥9 - Charpy U Notch
≥35
Bar, Coil; 20<d≤40 Quenching and Tempering 1030~1230 ≥830 ≥9 - ≥35
38CD4 Corresponding Standards(Same grade name, different standards)