Grade SCMnCr 3
Corresponding Standard JIS G 5111-1991
High tensile strength carbon steel castings and low alloy steel castings structural purposes
Classification Cast Steel
SCMnCr 3 Chemical Element Composition Content (%)
Component C Si Mn P S Cr
Minimum Value 0.3 0.3 1.2 - - 0.4
Maximum Value 0.4 0.6 1.6 0.04 0.04 0.8
SCMnCr 3 Mechanical Properties
condition Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Cast steel SCMnCr 3A Normalization Followed by Tempering ≥640 ≥390 ≥9 ≥25 ≥183
Cast steel SCMnCr 3B Quenching Followed by Tempering ≥690 ≥490 ≥13 ≥35 ≥207
Approximate Comparison Table Cast Steel
China Japan Russia
GB JIS GOST
ZG35CrMnSi SCMnCr3 35ХГСЛ