Grade 6181
Other Names
Corresponding Standard JIS H 4040-2015
Aluminium and Aluminium Alloy Bars and Wires
Classification Aluminum and Aluminum Alloys
Properties Corrosion Resistance
6181 Chemical Element Composition Content (%)
Component Fe Si Mn Cr Cu Ti Zn Mg Other Individual Other Total More
Minimum Value - 0.8 - - - - - 0.6 - - Al:余量
Maximum Value 0.45 1.2 0.15 0.1 0.1 0.1 0.2 1 0.05 0.15
"Other individual elements or other totals": The chemical composition includes elements not specified in the table. Analysis should only be conducted if these elements are suspected to be present, or if routine analysis suggests that their content may exceed the prescribed limits.
6181 Mechanical Properties
condition Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Cold-drawn bars (BD); d≤50 6181 T4 Solution Heat Treatment + Natural Aging (T4) ≥200 ≥100 A
≥15
Cold-drawn bars (BD); d≤50 6181 T6 Solid Solution Heat Treatment + Artificial Aging (T6) ≥280 ≥240 ≥8
① A50mm、A(5.65√S0)- gauge length,S0-Specimen area,s=S0,unit mm sq
② d-diameter、thickness or width across flats, unit mm;s - cross section area, unit mm sq
6181 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!