Grade C7541
Other Names
Corresponding Standard JIS H 3110-2018
Phosphor brozne and nickle silver sheets, plates and strips
Classification Copper and Copper Alloys
Properties Corrosion Resistance Fatigue Resistance
C7541 Chemical Element Composition Content (%)
Component Fe Mn Ni Cu Pb More
Minimum Value - - 12.5 60 - Zn:余量
Maximum Value 0.25 0.5 15.5 64 0.03
C7541 Mechanical Properties
condition Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Plate (P), strip (R); 0.1≤t≤5 C7541 P-O,C7541 R-O Annealing (O) ≥355 ≥20 -
Plate (P), strip (R); 0.1≤t≤5 C7541 P-1/2H,C7541 R-1/2H 1/2 Hard (1/2H) 410~540 ≥5 HV
110~170
Plate (P), Strip (R); 0.1≤t<0.15 C7541 P-H,C7541 R-H Hard (H) ≥490 - ≥135
Plate (P), Strip (R); 0.15≤t≤5 Hard (H) ≥490 ≥3 ≥135
Approximate Comparison Table Wrought Cupronickel
China Japan United States International Organization for Standardization Russia United Kingdom
GB ISC JIS ASTM UNS ISO Numerical Grade GOST Commercial Grade BS EN/BS
BZn15-20 T74600 C7541
C75400
63Cu-15Ni-22Zn C75400 CuNi15Zn21 C75400 МНЦ15-20 NS105 C75400
C7541 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!