Grade
1.1181
European Standard Steel Grade
C35E
Corresponding Standard
EN 10297-1-2003
Seamless steel tubes for mechanical and general engineering purposes - Technical delivery conditions - Part 1: Non-alloy and alloy steel tubes
Classification
Carbon Steel
1.1181 Chemical Element Composition Content (%)
Component
C
Si
Mn
P
S
Cr
Ni
Mo
Minimum Value
0.32
-
0.5
-
-
-
-
-
Maximum Value
0.39
0.4
0.8
0.035
0.035
0.4
0.4
0.1
1 Approximate Comparison Table
China
Taiwan, China
Japan
South Korea
United States
International Organization for Standardization
Germany
France
Russia
Sweden
United Kingdom
GB
ISC
CNS
JIS
KS
ASTM/AISI
UNS
ISO
DIN EN/DIN
W-Nr.
NF EN/NF
GOST
SS
BS EN/BS
35
U20352
S35C
S35C
SM35C
1035
G10350
C35E4
C35E
Ck35
1.1181
C35E
XC38
35
1572
C35E
080M36
2 Approximate Comparison Table
China
Japan
International Organization for Standardization
European Standard
GB
JIS
ISO
EN
Numerical Grade
35
S35C
C35E
C35E
1.1181
3 Approximate Comparison Table
China
Japan
United States
International Organization for Standardization
Germany
France
European Standard
Russia
Sweden
United Kingdom
GB
JIS
ASTM
ISO
DIN EN/DIN
NF EN/NF
EN
Numerical Grade
GOST
SS
BS EN/BS
35
S35C
1035
C35E4
Ck35
XC38
XC38H1
C35E
1.1181
35
1572
080M36
CFS6
4 Approximate Comparison Table
China
United States
International Organization for Standardization
European Standard
GB
ASTM/AISI
ISO
EN
Numerical Grade
35Mn
(GB/T 699-2015)
1037
(ASTM A29/A29M:2005)
C35E4
(ISO 683-18:1996)
C35E
(EN 10083-1:1991+A1:1996) (EN 10084:1998)
1.1181
1.1181 Corresponding Standards(Same grade name, different standards)
Message
I want to correct it
Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!