Grade 12CrNi3
China ISC A42122
Corresponding Standard GB /T 3077-2015
Alloy Structure Steels
Classification Alloy Steel
Properties Strength Weldability Carburizing Ability
Density 7.88 g/cm3
12CrNi3 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo
Minimum Value 0.1 0.17 0.3 - - 0.6 2.75 - -
Maximum Value 0.17 0.37 0.6 0.03 0.03 0.9 3.15 0.3 0.1
12CrNi3 Mechanical Properties
diameter
d
mmd
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
d=15 Double Quenching and Tempering ≥930 ≥685 ≥11 ≥50 ≤217 ≥71
Approximate Comparison Table Structural Alloy Steel
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France European Standard Russia United Kingdom
GB ISC CNS JIS KS ASTM/AISI UNS ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade GOST BS EN/BS
12CrNi3 A42122 SNC815 SNC815
SNC815H
SNC815 3310 G33106 15NiCr13 14NiCr14 1.5752 14NC12 15NiCr13 1.5752 12ХН3А 665A12
665M13
12CrNi3 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!