Grade C22R
1.1149
Old Grade
Corresponding Standard NF EN 10083-2-2006
Tempered non-alloy structural steel
Classification Carbon Steel
C22R Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo More
Minimum Value 0.17 - 0.4 - 0.02 - - - Cr+Mo+Ni≤0.63 ①
Maximum Value 0.24 0.4 0.7 0.03 0.04 0.4 0.4 0.1
C22R Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Impact Energy Absorption
KV2
J
Steel: d ≤ 16mm; t ≤ 8mm Quenching + Tempering (+QT) 500~650 ≥340 ≥20 ≥50
Steel: 16mm ≤ d ≤ 40mm; 8mm ≤ t ≤ 20mm Quenching + Tempering (+QT) 470~620 ≥290 ≥22 ≥50 ≥50
Steel: d ≤ 16mm; t ≤ 16mm Normalizing (+N) ≥430 ≥240 ≥24
Steel: 16mm ≤ d ≤ 100mm; 16mm ≤ t ≤ 100mm Normalizing (+N) ≥410 ≥210 ≥25
C22R Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!