Grade 28Mn6
1.1170
Corresponding Standard NF EN 10083-2-2006
Tempered non-alloy structural steel
Classification Carbon Steel
28Mn6 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo More
Minimum Value 0.25 - 1.3 - - - - - Cr+Mo+Ni≤0.63 ①
Maximum Value 0.32 0.4 1.65 0.03 0.035 0.4 0.4 0.1
28Mn6 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Steel: d ≤ 16mm; t ≤ 8mm Quenching + Tempering (+QT) 800~950 ≥590 ≥13 ≥40
Steel: 16mm ≤ d ≤ 40mm; 8mm ≤ t ≤ 20mm Quenching + Tempering (+QT) 700~850 ≥490 ≥15 ≥45 ≥40
Steel: 40mm ≤ d ≤ 100mm; 20mm ≤ t ≤ 60mm Quenching + Tempering (+QT) 650~800 ≥440 ≥16 ≥50 ≥40
Steel: d ≤ 16mm; t ≤ 16mm Normalizing (+N) ≥630 ≥345 ≥17
Steel: 16mm ≤ d ≤ 100mm; 16mm ≤ t ≤ 100mm Normalizing (+N) ≥600 ≥310 ≥18
Steel: 100mm ≤ d ≤ 250mm; 100mm ≤ t ≤ 250mm Normalizing (+N) ≥590 ≥290 ≥18
Steel: Processed to a Certain Shearability (+S) ≤255
Steel: Softening Annealing (+A) ≤223

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!