Grade 34Cr4
1.7033
Old Grade
Corresponding Standard NF EN 10083-3-2006
Tempered alloy structural steel
Classification Alloy Steel
34Cr4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr
Minimum Value 0.3 - 0.6 - - 0.9
Maximum Value 0.37 0.4 0.9 0.025 0.035 1.2
34Cr4 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Steel: d ≤ 16mm; t ≤ 8mm Quenching + Tempering (+QT) 900~1100 ≥700 ≥12 ≥35
Steel: 16mm ≤ d ≤ 40mm; 8mm ≤ t ≤ 20mm Quenching + Tempering (+QT) 800~950 ≥590 ≥14 ≥40 ≥40
Steel: 40mm ≤ d ≤ 100mm; 20mm ≤ t ≤ 60mm Quenching + Tempering (+QT) 700~850 ≥460 ≥15 ≥45 ≥40
Steel: Processed to a Certain Shearability (+S) ≤255
Steel: Softening Annealing (+A) ≤223

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!