30CrNiMo8 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo
Minimum Value 0.26 - 0.5 - - 1.8 1.8 0.3
Maximum Value 0.34 0.4 0.8 0.025 0.035 2.2 2.2 0.5
30CrNiMo8 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Steel: d ≤ 16mm; t ≤ 8mm Quenching + Tempering (+QT) 1250~1450 ≥1050 ≥9 ≥40
Steel: 16mm ≤ d ≤ 40mm; 8mm ≤ t ≤ 20mm Quenching + Tempering (+QT) 1250~1450 ≥1050 ≥9 ≥40 ≥30
Steel: 40mm ≤ d ≤ 100mm; 20mm ≤ t ≤ 60mm Quenching + Tempering (+QT) 1000~1300 ≥900 ≥10 ≥45 ≥35
Steel: 100mm ≤ d ≤ 160mm; 60mm ≤ t ≤ 100mm Quenching + Tempering (+QT) 1000~1200 ≥800 ≥11 ≥50 ≥45
Steel: 160mm ≤ d ≤ 250mm; 100mm ≤ t ≤ 160mm Quenching + Tempering (+QT) 900~1100 ≥700 ≥12 ≥50 ≥45
Steel: Processed to a Certain Shearability (+S)
Steel: Softening Annealing (+A) ≤248