Grade 27MnCrB5-2
1.7182
Corresponding Standard NF EN 10083-3-2006
Steels for Quenching and Tempering - Part 3: Technical Delivery Conditions for Alloy Steels
Classification Alloy Steel
27MnCrB5-2 Chemical Element Composition Content (%)
Component C Si Mn P S Cr B
Minimum Value 0.24 - 1.1 - - 0.3 0.0008
Maximum Value 0.3 0.4 1.4 0.025 0.035 0.6 0.005
27MnCrB5-2 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Steel: d ≤ 16mm; t ≤ 8mm Quenching + Tempering (+QT) 1000~1250 ≥800 ≥14 ≥55
Steel: 16mm ≤ d ≤ 40mm; 8mm ≤ t ≤ 20mm Quenching + Tempering (+QT) 900~1150 ≥750 ≥14 ≥55 ≥60
Steel: 40mm ≤ d ≤ 100mm; 20mm ≤ t ≤ 60mm Quenching + Tempering (+QT)
800~1000

≥700

≥15

≥55

≥65
Steel: Processed to a Certain Shearability (+S)
Steel: Softening Annealing (+A)
27MnCrB5-2 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!