Grade 1Cr17Ni8
Corresponding Standard GB /T 4239-1991
Cold Rolled Stainless Steel and Heat-Resisting Steel Strip
Classification Austenitic Stainless Steel
Properties Corrosion Resistance
1Cr17Ni8 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni
Minimum Value 0.08 - - - - 16 7
Maximum Value 0.12 1 2 0.035 0.03 18 9
1Cr17Ni8 Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Solid Solution Treatment ≥570 ≥205 ≥45 HRB ≤90;HV ≤200
Approximate Comparison Table Austenitic Stainless Steel
China Japan Germany
GB JIS DIN EN/DIN
1Cr17Ni8 SUS301J1 X12CrNi17-7

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!