Grade 30Cr2Ni4Mo
China ISC A50300
Corresponding Standard GB /T 3077-2015
Alloy structure steels
Classification Alloy Steel
Properties Strength Quench Hardness
30Cr2Ni4Mo Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo
Minimum Value 0.26 0.17 0.5 - - 1.2 3.3 - 0.3
Maximum Value 0.33 0.37 0.8 0.03 0.03 1.5 4.3 0.3 0.6
30Cr2Ni4Mo Mechanical Properties
diameter
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
d=25 Quenching + Tempering ≥1080 ≥930 ≥10 ≥50 ≤269 ≥71
1 Approximate Comparison Table Alloy Steel for Quenching and Tempering
China Japan International Organization for Standardization Germany European Standard
GB ISC JIS ISO DIN EN/DIN W-Nr. EN Numerical Grade
30Cr2Ni2Mo A50300 SNCM431 30CrNiMo8 30CrNiMo8 1.6580 30CrNiMo8 1.6580
2 Approximate Comparison Table Structural Alloy Steel
China Germany European Standard United Kingdom
GB DIN EN/DIN W-Nr. EN Numerical Grade BS EN/BS
30Cr2Ni4Mo 30NiCrMo16-6 1.6747 30NiCrMo16-6 1.6747 835M30

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!