Grade Cm60
Germany W-Nr. 1.1223
Corresponding Standard DIN 17204-1990
Seamless circular tubes made from steels for quenching and tempering Technical delivery conditions
Classification Carbon Steel
Cm60 Chemical Element Composition Content (%)
Component C Si Mn P S
Minimum Value 0.57 - 0.6 - 0.02
Maximum Value 0.65 0.4 0.9 0.035 0.035
Cm60 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Hot drawn, cold drawn pipes Annealing ≤241
Pipe material t≤16 Normalizing (N) 720~900 ≥390 ≥13(long.);≥11(tr.)
Pipe material 16<t≤40 Normalizing (N) 700~880 ≥370 ≥14(long.);≥12(tr.)
Pipe material 40<t≤80 Normalizing (N) 670~850 ≥360 ≥14(long.);≥12(tr.)
Pipes t≤8 Quenching + Tempering (V) 850~1050 ≥580 ≥11(long.);≥9(tr.) ≥25
Pipes; 8< t≤20 Quenching + Tempering (V) 800~1000 ≥520 ≥13(long.);≥11(tr.) ≥30
Pipes; 20< t≤50 Quenching + Tempering (V) 750~950 ≥450 ≥14(long.);≥12(tr.) ≥35
Pipe; 50<t≤80 Quenching + Tempering (V) 710~910 ≥420 ≥14(long.);≥12(tr.) ≥35
Approximate Comparison Table Non-Alloy Steel for Quenching and Tempering
International Organization for Standardization Germany European Standard
ISO DIN EN/DIN EN Numerical Grade
C60R
C60M2
Cm60 C60R 1.1223
Cm60 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!