Grade 7CrMoVTiB10-10
1.7378
Corresponding Standard NF EN 10216-2-2007
Pressurized seamless steel tubes for high temperatures
Classification Alloy Steel
7CrMoVTiB10-10 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Mo N Ti V B Al
Minimum Value 0.05 0.15 0.3 - - 2.2 0.9 - 0.05 0.2 0.0015 -
Maximum Value 0.1 0.45 0.7 0.02 0.01 2.6 1.1 0.01 0.1 0.3 0.007 0.02
◎ Elements not included in this table shall not be intentionally added to the steel without the agreement of the purchaser, except for elements which may be added for finishing the cast. All appropriate measures shall be taken to prevent the addition of undesirable elements from scrap or other materials used in the steel making process.
7CrMoVTiB10-10 Mechanical Properties
thickness
T
mm
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
Steel: T ≤ 16 565~840 ≥450 l ≥17;t≥15 20℃:l ≥ 40,t≥27
Steel: 16 < T ≤ 40 565~840 ≥430 l ≥17;t≥15 20℃:l ≥ 40,t≥27
Steel: 40 < T ≤ 60 565~840 ≥430 (applicable to wall thickness T ≤ 50mm) l ≥17;t≥15 20℃:l ≥ 40,t≥27
◎ l-longitudinal;t-transverse