Grade CuZn37Al1
Germany W-Nr. 2.0510
Old Grade
Corresponding Standard DIN 17672-1-1983
Wrought copper and copper alloys bars;Properties.
Classification Copper and Copper Alloys
Density 8.3 g/cm3
CuZn37Al1 Chemical Element Composition Content (%)
Component Fe Si Mn Ni Cu Pb Al Sn Other Total More
Minimum Value - - 0.6 - 59 - 0.3 - - Zn:余量
Maximum Value 1 0.5 1.8 0.6 61.5 1 1.3 0.3 0.5
"Other individual elements or other totals": The chemical composition includes elements not specified in the table. Analysis should only be conducted if these elements are suspected to be present, or if routine analysis suggests that their content may exceed the prescribed limits.
CuZn37Al1 Mechanical Properties
diameter/thickness
d
mm
Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Round profiles; 10≤d<80 2.0510.27 Semi-Hard + Stress Relief F44 (.27) ≥440 ≥200 ≥20(A5) ≈125
Square, hexagonal profiles; 9≤d<70 2.0510.27 Semi-Hard + Stress Relief F44 (.27) ≥440 ≥200 ≥20(A5) ≈125
Round material; 6 ≤ d < 50 2.0510.31 Hard + Stress Relief F51 (.31) ≥510 ≥280 ≥15(A5) ≈145
Square material, hexagonal material; 5 ≤ d < 46 2.0510.31 Hard + Stress Relief F51 (.31) ≥510 ≥280 ≥15(A5) ≈145
Approximate Comparison Table Cupper and cupper alloy
Germany European Standard
DIN EN/DIN W-Nr. EN Numerical Grade
CuZn37Al2 2.0510 CuZn38Mn1Al CW716R
CuZn37Al1 Corresponding Standards(Same grade name, different standards)