Grade X2CrNiMo17-12-2
1.4404
Corresponding Standard NF EN 10088-2-2005
Part2:Technical delivery conditions for sheet/plate and strip of corrosion resisting steels for general purposes
Classification Austenitic Stainless Steel
X2CrNiMo17-12-2 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N
Minimum Value - - - - - 16.5 10 2 -
Maximum Value 0.03 1 2 0.045 0.015 18.5 13 2.5 0.11
◎ Elements not listed in this table shall not be intentionally added to the steel without the agreement of the purchaser except for finishing the cast. All appropriate precautions are to be taken to avoid the addition of such elements from scrap and other materials used in production which would impair mechanical properties and the suitability of the steel.
X2CrNiMo17-12-2 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
Cold rolled strip steel: T ≤ 8mm +AT 530~680 ( t )
Rp0.2:≥ 240①③
Rp1.0:≥ 270①②
( t )
T<3mm:≥40③④
T ≥ 3mm:≥40③⑤
-
Hot rolled strip steel: T ≤ 13.5mm +AT 530~680 ( t )
Rp0.2:≥ 220①③
Rp1.0:≥ 260①②
( t )
T<3mm:≥40③④
T ≥ 3mm:≥40③⑤
(T>10mm)
I:≥ 100;t:≥60
Hot rolled medium and thick plates: T ≤ 75mm +AT 520~670 ( t )
Rp0.2:≥ 220①③
Rp1.0:≥ 260①②
( t )
T<3mm:≥45③④
T ≥ 3mm:≥45③⑤
(T>10mm)
I:≥ 100;t:≥60
◎ T-thickness;l-longitudinal;t-trasverse
◎ +A=soft annealed;+QT=quenched and tempered;+P=precipitation hardened;+AT=solutiong annealed;+SR=strength relieved

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!