Grade X2CrNiMoN18-12-4
1.4434
Corresponding Standard NF EN 10088-2-2005
Part2:Technical delivery conditions for sheet/plate and strip of corrosion resisting steels for general purposes
Classification Austenitic Stainless Steel
X2CrNiMoN18-12-4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N
Minimum Value - - - - - 16.5 10.5 3 0.1
Maximum Value 0.03 1 2 0.045 0.015 19.5 14 4 0.2
◎ Elements not listed in this table shall not be intentionally added to the steel without the agreement of the purchaser except for finishing the cast. All appropriate precautions are to be taken to avoid the addition of such elements from scrap and other materials used in production which would impair mechanical properties and the suitability of the steel.
X2CrNiMoN18-12-4 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
Cold rolled strip steel: T ≤ 8mm +AT 570~770 ( t )
Rp0.2:≥ 290①③
Rp1.0:≥ 320①②
( t )
T<3mm:≥35③④
T ≥ 3mm:≥35③⑤
-
Hot rolled strip steel: T ≤ 13.5mm +AT 570~770 ( t )
Rp0.2:≥ 270①③
Rp1.0:≥ 310①②
( t )
T<3mm:≥35③④
T ≥ 3mm:≥35③⑤
(T>10mm)
I:≥ 100;t:≥60
Hot rolled medium and thick plates: T ≤ 75mm +AT 540~740 ( t )
Rp0.2:≥ 270①③
Rp1.0:≥ 310①②
( t )
T<3mm:≥40③④
T ≥ 3mm:≥40③⑤
(T>10mm)
I:≥ 100;t:≥60
◎ T-thickness;l-longitudinal;t-trasverse
◎ +A=soft annealed;+QT=quenched and tempered;+P=precipitation hardened;+AT=solutiong annealed;+SR=strength relieved
Approximate Comparison Table
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France European Standard
GB ISC CNS JIS KS ASTM UNS ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade
022Cr19Ni13Mo4N S31753 317LN SUS 317LN STS 317LN 317LN S31753 X2CrNiMoN 18-12-4 X2CrNiMoN 18-12-4 1.4434 X2CrNiMoN 18-12-4 X2CrNiMoN 18-12-4 1.4434

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!