Grade X2CrNiMoN22-5-3
1.4462
Corresponding Standard NF EN 10088-2-2005
Part2:Technical delivery conditions for sheet/plate and strip of corrosion resisting steels for general purposes
Classification Duplex Stainless Steel
X2CrNiMoN22-5-3 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N
Minimum Value - - - - - 21 4.5 2.5 0.1
Maximum Value 0.03 1 2 0.035 0.015 23 6.5 3.5 0.22
◎ Elements not listed in this table shall not be intentionally added to the steel without the agreement of the purchaser except for finishing the cast. All appropriate precautions are to be taken to avoid the addition of such elements from scrap and other materials used in production which would impair mechanical properties and the suitability of the steel.
X2CrNiMoN22-5-3 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
Cold rolled strip steel: T ≤ 8mm +AT 700~950 t:≥ 500①② T<3mm:≥20
T ≥ 3mm:≥20 ③
-
Hot rolled strip steel: T ≤ 13.5mm +AT 700~950 t:≥ 460①② T<3mm:≥25
T ≥ 3mm:≥25
(T>10mm)
I:≥ 100;t:≥60
Hot rolled medium-thick plate: T ≤ 75mm④ +AT 640~840 t:≥ 460①② T<3mm:≥25
T ≥ 3mm:≥25
(T>10mm)
I:≥ 100;t:≥60
◎ T-thickness;l-longitudinal;t-trasverse
◎ +A=soft annealed;+QT=quenched and tempered;+P=precipitation hardened;+AT=solutiong annealed;+SR=strength relieved
Approximate Comparison Table
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France European Standard
GB ISC CNS JIS KS UNS ISO Numerical Grade DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade
022Cr22Ni5Mo3N
022Cr23Ni5Mo3N
S22253
S22053
329J3L SUS 329J3L STS 329J3L S31803
S32205
X2CrNiMoN 22-5-3 4462-318-03-I X2CrNiMoN 22-5-3 1.4462 X2CrNiMoN 22-5-3 X2CrNiMoN 22-5-3 1.4462

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!