Grade X2CrNiMoCuN25-6-3
1.4507
Corresponding Standard NF EN 10088-2-2005
Part2:Technical delivery conditions for sheet/plate and strip of corrosion resisting steels for general purposes
Classification Duplex Stainless Steel
X2CrNiMoCuN25-6-3 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo N
Minimum Value - - - - - 24 6 1 3 0.2
Maximum Value 0.03 0.7 2 0.035 0.015 26 8 2.5 4 0.3
◎ Elements not listed in this table shall not be intentionally added to the steel without the agreement of the purchaser except for finishing the cast. All appropriate precautions are to be taken to avoid the addition of such elements from scrap and other materials used in production which would impair mechanical properties and the suitability of the steel.
X2CrNiMoCuN25-6-3 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
Cold rolled strip steel: T ≤ 8mm +AT 750~1000 t:≥ 550①② T<3mm:≥20
T ≥ 3mm:≥20 ③
-
Hot rolled strip steel: T ≤ 13.5mm +AT 750~1000 t:≥ 530①② T<3mm:≥20
T ≥ 3mm:≥20 ③
(T>10mm)
I:≥ 100;t:≥60
Hot rolled medium-thick plate: T ≤ 75mm④ +AT 730~930 t:≥ 530①② T<3mm:≥25
T ≥ 3mm:≥25 ③
(T>10mm)
I:≥ 100;t:≥60
◎ T-thickness;l-longitudinal;t-trasverse
◎ +A=soft annealed;+QT=quenched and tempered;+P=precipitation hardened;+AT=solutiong annealed;+SR=strength relieved
Approximate Comparison Table
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France European Standard
GB ISC CNS JIS KS ASTM/AISI UNS ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade
03Cr25Ni6Mo3Cu2N S25554 329J4L SUS 329J4L STS 329J4L 255 S32550 X2CrNiMoCuN 25-6-3 X2CrNiMoCuN 25-6-3 1.4507 X2CrNiMoCuN 25-6-3 X2CrNiMoCuN 25-6-3 1.4507

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!