Grade 36SMnPb14
1.0765
Corresponding Standard NF EN 10087-1999
Free-cutting structural steels
Classification Carbon Steel
36SMnPb14 Chemical Element Composition Content (%)
Component C Si Mn P S Pb
Minimum Value 0.32 - 1.3 - 0.1 0.15
Maximum Value 0.39 0.4 1.7 0.06 0.18 0.35
36SMnPb14 Mechanical Properties
diameter
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Steel: 5≤ d ≤10 Untreated State 580~770
Steel: 10<d ≤16 Untreated State 580~770
Steel: 16 < d ≤ 40 Untreated State 560~750 166~222
Steel: 40 < d ≤ 63 Untreated State 560~740 166~219
Steel: 63 < d ≤ 100 Untreated State 550~740 166~219
Steel: 5≤ d ≤10 Quenching + Tempering (+QT) 700~850 ≥480 ≥14
Steel: 10<d ≤16 Quenching + Tempering (+QT) 700~850 ≥460 ≥14
Steel: 16 < d ≤ 40 Quenching + Tempering (+QT) 670~820 ≥420 ≥15
Steel: 40 < d ≤ 63 Quenching + Tempering (+QT) 640~790 ≥400 ≥16
Steel: 63 < d ≤ 100 Quenching + Tempering (+QT) 570~720 ≥360 ≥17

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!