Grade Ni99.6
Germany W-Nr. 2.4060
Corresponding Standard DIN 17752-2002
Wrought nickel and nickel alloy rod and bars Requirements and testing
Classification Nickel and Nickel Alloys
Properties Corrosion Resistance
Density 8.9 g/cm3
Ni99.6 Chemical Element Composition Content (%)
Component Fe C Si Mn S Cu Ti Co Mg More
Minimum Value - - - - - - - - - Ni+Co≥99.6
Maximum Value 0.25 0.08 0.15 0.35 0.005 0.15 0.1 1 0.15
Ni99.6 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Rods; 2≤d≤55 Soft annealing (F37) ≥370 ≥100 ≥40 ≤130 HBW2.5/62.5
Bar stock; 2≤d≤50 1/2-Hard (F49) ≥490 ≥340 ≥15 ≈150 HBW2.5/62.5
Bars; 2 ≤ d ≤ 35 Hard (F59) ≥590 ≥540 ≥5 ≈200 HBW2.5/62.5
Approximate Comparison Table Corrosion-Resistant Alloy
China United States Germany
GB ISC Commercial Grade UNS W-Nr.
NS 5200
N5
H 02200 Nickel 200 N 02200 2.4060
Ni99.6 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!