Grade CuSn4
Germany W-Nr. CW450K
Corresponding Standard DIN EN 12166-2016
Copper and copper alloys – Wire for general purposes
Classification Copper and Copper Alloys
Density 8.9 g/cm3
CuSn4 Chemical Element Composition Content (%)
Component Fe P Ni Pb Zn Sn Other Total More
Minimum Value - 0.01 - - - 3.5 - Cu:余量
Maximum Value 0.1 0.4 0.2 0.02 0.2 4.5 0.2
"Other individual elements or other totals": The chemical composition includes elements not specified in the table. Analysis should only be conducted if these elements are suspected to be present, or if routine analysis suggests that their content may exceed the prescribed limits.
CuSn4 Mechanical Properties
diameter*
d
mm
Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
1.5<d≤20 CuSn4-H085 H085 HV
85~115
1.5<d≤12 CuSn4-H125 H125 125~155
1.5<d≤8 CuSn4-H150 H150 150~185
1.5<d≤4 CuSn4-H210 H210 ≥210
d≤1.5 CuSn4-H230 H230 ≥230
1.5<d≤20 CuSn4-R330 R330 ≥330 ≤220 ≥35(A100),
≥40(A11.3),
≥45(A)
0.1<d≤12 CuSn4-R420 R420 ≥420 ≥220 ≥20(A100),
≥25(A11.3),
≥30(A)
0.1<d≤8 CuSn4-R520 R520 ≥520 ≥380 ≥5(A100),
≥6(A11.3)
0.1<d≤4 CuSn4-R650 R650 ≥650 ≥500
0.1<d≤1.5 CuSn4-R850 R850 ≥850 ≥750
All specifications CuSn4-M M No specification No specification No specification No specification
1 Approximate Comparison Table bronze
China United States International Organization for Standardization Germany European Standard Russia
GB ISC ASTM UNS ISO Numerical Grade DIN EN/DIN W-Nr. EN Numerical Grade GOST
QSn4-0.3 C51100 96Cu-4Sn-.2P C51100 CuSn4 C51100 CuSn4 2.1016
C51100
CuSn4 CW450K БрОФ4-0.25
2 Approximate Comparison Table Cupper and cupper alloy
Germany European Standard
DIN EN/DIN W-Nr. EN Numerical Grade
CuSn4 2.1016 CuSn4 CW450K
CuSn4 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!