Grade 37Mn
Corresponding Standard GB /T 18248-2021
Seamless Steel Tubes for Gas Cylinder
Classification Carbon Steel
37Mn Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Al More
Minimum Value 0.34 0.1 1.35 - - - - - 0.02 P+S≤0.025;V+Nb+Ti+B+Zr≤0.15ⓐ
Maximum Value 0.38 0.35 1.75 0.02 0.01 0.3 0.3 0.2 -
37Mn Mechanical Properties
condition Test Temperature Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
Steel pipe specimen Room Temperature 820~860°C Quenching (Normalizing), Water Cooling + 550~650°C Tempering, Air Cooling ≥750 ≥630 ≥16 ≥27(-50°C)
Steel pipe specimen Room Temperature 830~870°C Quenching (Normalizing), Air Cooling ≥700 ≥520 ≥16 ≥27(-20°C)
Steel pipe specimen Room Temperature Normalizing ≥700 ≥520 ≥20①
Steel pipe specimen Room Temperature Tempering ≥730 ≥610 ≥14②
Steel Pipe Outer Diameter D>140mm; t=3*~10, Transverse Normalizing ≥20③;≥16④
Steel pipe outer diameter D≤140mm; t=3~10, Longitudinal Normalizing ≥40③;≥32④
Steel Pipe Outer Diameter D>140mm; t=3*~5, Transverse Tempering ≥30③;≥24④
Steel Pipe Outer Diameter D>140mm; t=5~7.5, Transverse Tempering ≥35③;≥28④
Steel Pipe Outer Diameter D>140mm; t=7.5~10, Transverse Tempering ≥40③;≥32④
Steel pipe outer diameter D≤140mm; t=3~10, Longitudinal Tempering ≥60③;≥48④

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!