Grade X3CrNiMoN 27-5-2
European Standard Steel Grade 1.4460
Corresponding Standard EN 10250-4-1999
Classification Duplex Stainless Steel
Properties Corrosion Resistance
Density 7.8 g/cm3
X3CrNiMoN 27-5-2 Chemical Element Composition Content (%)
Component C Si Mn P S * Cr Ni Mo N
Minimum Value - - - - - 25 4.5 1.3 0.05
Maximum Value 0.05 1 2 0.035 0.03 28 6.5 2 0.2
* For products to be machined a controlled sulfur content of 0.015% to 0.030% is recommended.
X3CrNiMoN 27-5-2 Mechanical Properties
diameter
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤160* Solid Solution Annealing 620~880 ≥460 longitudinal: ≥20
transverse: ≥15
longitudinal: ≥85
transverse: ≥50
Approximate Comparison Table
China United States International Organization for Standardization Germany France European Standard
GB ISC UNS ISO Numerical Grade DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade
022Cr25Ni6Mo2N S22553 S31200 X3CrNiMoN 27-5-2 4460-312-00-I X3CrNiMoN 27-5-2 1.4460 X3CrNiMoN 27-5-2 X3CrNiMoN 27-5-2 1.4460

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!