Grade CuZn40Pb2
Germany W-Nr. CW617N
Corresponding Standard DIN EN 12166-1998
Copper and copper alloys – Wire for general purposes
Classification Copper and Copper Alloys
Density 8.4 g/cm3
CuZn40Pb2 Chemical Element Composition Content (%)
Component Fe Ni Cu Pb Al Sn Other Total More
Minimum Value - - 57 1.6 - - - Zn:余量
Maximum Value 0.3 0.3 59 2.5 0.05 0.3 0.2
"Other individual elements or other totals": The chemical composition includes elements not specified in the table. Analysis should only be conducted if these elements are suspected to be present, or if routine analysis suggests that their content may exceed the prescribed limits.
CuZn40Pb2 Mechanical Properties
diameter③
d
mm
Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
0.5≤d≤1.5 CuZn40Pb2-R450 1/2 Hard; R450 ≥450 ≈200*
1.5<d≤4 CuZn40Pb2-R430 1/2 Hard; R430 ≥430 ≈200* ≥6(A100)
1.5≤d≤4 CuZn40Pb2-H130 1/2 Hard; H130 HV: 130~165
4<d≤8 CuZn40Pb2-R420 1/2 Hard; R420 ≥420 ≈200* ≥8(A11.3)
4<d≤8 CuZn40Pb2-H120 1/2 Hard; H120 HV: 120~155
8<d≤14 CuZn40Pb2-R410 1/2 Hard; R410 ≥410 ≈200* ≥10(A)
14<d≤20 CuZn38Pb4-R400 1/2 Hard; R400 ≥400 ≈200* ≥10(A)
8<d≤20 CuZn40Pb2-H110 1/2 Hard; H110 HV: 110~145
0.5≤d≤1.5 CuZn40Pb2-R520 Hard; R520 ≥520 ≈400*
1.5<d≤4 CuZn38Pb4-R510 Hard; R510 ≥510 ≈400* ≥4*(A100)
1.5≤d≤4 CuZn40Pb2-H155 Hard; H155 HV: 155~185
4<d≤8 CuZn40Pb2-R500 Hard; R500 ≥500 ≈390* ≥6(A11.3)
8<d≤14 CuZn40Pb2-R490 Hard; R490 ≥490 ≈390* ≥8(A)
4<d≤14 CuZn40Pb2-H145 Hard; H145 HV: 145~175
1.5≤d≤4 CuZn40Pb2-R570 Tough and Hard; R570 ≥570 ≈520*
1.5≤d≤4 CuZn40Pb2-H170 Tough Hard; H170 HV: ≥170
All specifications CuZn40Pb2-M M No specification No specification No specification No specification
① Material status name and character code: H-hardness (Brinell hardness or Vickers hardness), suffix number indicates the hardness value; R- tensile strength, suffix number indicates the minimum tensile strength value; M- When manufactured, no mechanical properties are specified. See standard EN 1173-2008.
② A100、A11.3、A-gauge length
—Value when the gauge length A100 = 100 mm (d < 4mm).
—Value When the gauge length A = 5.65√So (d > 8mm); When the gauge length A11.3 = 11.3√So (4 < d ≤ 8mm), the minimum elongation value is 40%.
—Value when the gauge length A = 5.65√So (d > 8mm); When the gauge length A11.3 = 11.3√So (4 < d ≤ 8mm), the minimum elongation value is 20%.
—The value when the gauge length A11.3 = 11.3√So (4 < d ≤ 8mm). (See original 8.2Note2 for the above spacing)
Tables such as: softened, 1/8 hard, spring hard, etc., refer to the state of the material in the old standard
③ Or equivalent cross-sectional area for polygonal wire
1 Approximate Comparison Table Brass
China Japan United States International Organization for Standardization Germany European Standard Russia
GB ISC JIS ASTM UNS ISO Numerical Grade DIN EN/DIN W-Nr. EN Numerical Grade GOST
HPb58-2 T38210 C3801
C38000
58Cu-40Zn-2Pb C38000 CuZn40Pb2 C38000 CuZn40Pb2 C38000
2.0402
CuZn40Pb2 CW617N ЛС58-2
2 Approximate Comparison Table Copper and Copper Alloy
Japan United States International Organization for Standardization Germany France European Standard Sweden United Kingdom
JIS UNS ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade SS BS EN/BS
C3771 C37700 CuZn40Pb2 CuZn39Pb2
CuZn40Pb2
2.0380 CuZn39Pb2 CuZn39Pb2 CW612N CuZn40Pb2 CZ120
3 Approximate Comparison Table Copper and Copper Alloy
Germany European Standard Russia
DIN EN/DIN W-Nr. EN Numerical Grade GOST
CuZn40Pb2 2.0402 CuZn40Pb2 CW617N LS59-2

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!