Grade Z20NCS33-16
Corresponding Standard NF A 35-578-1991
Iron and Steel. Stainless Steel for High Temperature Application
Classification Austenitic Stainless Steel
Z20NCS33-16 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni
Minimum Value - 1 - - - 14 32
Maximum Value 0.2 2 0.5 0.035 0.015 17 34
Z20NCS33-16 Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
+Q1050~1100 550~800 ≥230 ≥30 ≤223

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!