Grade CuZn37Pb1Sn1
European Standard Steel Grade CW714R
Corresponding Standard EN 12166-1998
Copper and copper alloys — Wire for general purposes
Classification Copper and Copper Alloys
Density 8.4 g/cm3
CuZn37Pb1Sn1 Chemical Element Composition Content (%)
Component Fe Ni Cu Pb Sn Other Total More
Minimum Value - - 59 0.4 0.5 - Zn:余量
Maximum Value 0.1 0.3 61 1 1 0.2
"Other individual elements or other totals": The chemical composition includes elements not specified in the table. Analysis should only be conducted if these elements are suspected to be present, or if routine analysis suggests that their content may exceed the prescribed limits.
CuZn37Pb1Sn1 Mechanical Properties
diameter③
d
mm
Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
0.1≤d≤20 CuZn37Pb1Sn1-R350 R350 350~450 ≥15(A100),
≥18(A11.3),
≥20(A)
0.1≤d≤20 CuZn37Pb1Sn1-H100 H100 HV: 100~130
1.5≤d≤8 CuZn37Pb1Sn1-R400 R400 ≥400 ≥10(A100),
≥13(A11.3)
1.5≤d≤8 CuZn37Pb1Sn1-H120 H120 HV: ≥120
All specifications CuZn37Pb1Sn1-M M No specification No specification No specification No specification
①Material condition designation: H-Hardness (Brinell or Vickers), the suffix number indicates the hardness value; R-Tensile strength, the suffix number indicates the minimum tensile strength; M-As manufactured, without specified mechanical properties
②A100, A11.3, A-gauge length
③Or equivalent cross-sectional area for polygonal wire.
CuZn37Pb1Sn1 Corresponding Standards(Same grade name, different standards)