USA UNS S20910
ASTM
Specification or Grade
XM-19
Corresponding Standard ASTM A479/A479M-2018
Standard Specification for Stainless Steel Bars and Shapes for Use in Boilers and Other Pressure Vessels
Classification Austenitic Stainless Steel
Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N V Cb
Minimum Value - - 4 - - 20.5 11.5 1.5 0.2 0.1 0.1
Maximum Value 0.06 1 6 0.045 0.03 23.5 13.5 3 0.4 0.3 0.3
◎ New designations established in accordance with Practice E527 and SAE J1086 published jointly by ASTM and SAE. See ASTM DS-56C, available from ASTM Headquarters.
Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
All specifications Annealing ≥690 ≥380 in 2 in.[50 mm] or 4D
≥ 35
≥ 55 ① ≤293
d ≤ 50.8mm Hot Rolling ≥930 ≥725 in 2 in.[50 mm] or 4D
≥ 20
≥ 50 ① -
50.8mm <d ≤ 76.2mm Hot Rolling ≥795 ≥515 in 2 in.[50 mm] or 4D
≥ 25
≥ 50 ① -
76.2mm <d ≤ 203.2mm Hot Rolling ≥690 ≥415 in 2 in.[50 mm] or 4D
≥ 30
≥ 50 ① -
d ≤ 38.1mm Strain hardening ≥1000 ≥860 in 2 in.[50 mm] or 4D
≥ 12
≥ 40 ① -
38.1mm <d ≤ 57.2mm Strain hardening ≥825 ≥725 in 2 in.[50 mm] or 4D
≥ 15
≥ 45 ① -
◎ d-diameter, t-thickness

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!