USA UNS S21600
ASTM
Specification or Grade
XM-17
Corresponding Standard ASTM A479/A479M-2018
Standard Specification for Stainless Steel Bars and Shapes for Use in Boilers and Other Pressure Vessels
Classification Austenitic Stainless Steel
Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N
Minimum Value - - 7.5 - - 17.5 5 2 0.25
Maximum Value 0.08 1 9 0.045 0.03 20.5 7 3 0.5
◎ New designations established in accordance with Practice E527 and SAE J1086 published jointly by ASTM and SAE. See ASTM DS-56C, available from ASTM Headquarters.
Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
All specifications Annealing ≥620 ≥345 in 2 in.[50 mm] or 4D
≥ 40
≥ 50 ① ≤212
◎ d-diameter, t-thickness

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!