USA UNS S35315
Corresponding Standard ASTM A479/A479M-2018
Standard Specification for Stainless Steel Bars and Shapes for Use in Boilers and Other Pressure Vessels
Classification Austenitic Stainless Steel
Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni N Ce
Minimum Value 0.04 1.2 - - - 24 34 0.12 0.03
Maximum Value 0.08 2 2 0.04 0.03 26 36 0.18 0.08
◎ New designations established in accordance with Practice E527 and SAE J1086 published jointly by ASTM and SAE. See ASTM DS-56C, available from ASTM Headquarters.
Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
All specifications Annealing ≥650 ≥270 in 2 in.[50 mm] or 4D
≥ 40
◎ d-diameter, t-thickness
Approximate Comparison Table Austenitic Stainless Steel
United States International Organization for Standardization European Standard
UNS ISO Numerical Grade EN Numerical Grade
S35315 X6NiCrSiNCe35-25 4854-353-15-E X6NiCrSiNCe35-25 1.4854