Grade 7075
Corresponding Standard SAE AMS4045M-2000(R2022)
Aluminum Alloy Sheet and Plate 5.6Zn - 2.5Mg - 1.6Cu - 0.23Cr 7075: (-T6 Sheet, -T651 Plate) Solution and Precipitation Heat Treated
Classification Aluminum and Aluminum Alloys
7075 Chemical Element Composition Content (%)
Component Fe Si Mn Cr Cu Ti Zn Mg Other Individual Other Total More
Minimum Value - - - 0.18 1.2 - 5.1 2.1 - - Al余量
Maximum Value 0.5 0.4 0.3 0.28 2 0.2 6.1 2.9 0.05 0.15
"Other individual elements or other totals": The chemical composition includes elements not specified in the table. Analysis should only be conducted if these elements are suspected to be present, or if routine analysis suggests that their content may exceed the prescribed limits.
7075 Mechanical Properties
thickness
t
mm
Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
0.2<t≤0.28 7075-T6
7075T651
T6;T651 ≥510 ≥434 ≥5
0.28<t≤0.99 7075-T6
7075T651
T6;T651 ≥524 ≥462 ≥8
0.99<t≤3.18 7075-T6
7075T651
T6;T651 ≥538 ≥469 ≥9
3.18<t≤4.75 7075-T6
7075T651
T6;T651 ≥545 ≥476 ≥9
4.75<t≤6.32 7075-T6
7075T651
T6;T651 ≥552 ≤476 ≥9
6.32<t≤12.67 7075-T6
7075T651
T6;T651 ≥538 ≥462 ≥9
12.67<t≤25.4 7075-T6
7075T651
T6;T651 ≥538 ≥469 ≥7
25.4<t≤50.8 7075-T6
7075T651
T6;T651 ≥531 ≥462 ≥6
50.8<t≤63.5 7075-T6
7075T651
T6;T651 ≥524 ≥441 ≥5
63.5<t≤76.2 7075-T6
7075T651
T6;T651 ≥496 ≥421 ≥5
76.2<t≤88.9 7075-T6
7075T651
T6;T651 ≥490 ≥400 ≥5
88.9<t≤101.6 7075-T6
7075T651
T6;T651 ≥462 ≥372 ≥3
Approximate Comparison Table Wrought aluminum and aluminum alloy
China United States International Organization for Standardization Germany European Standard Australia
ISC ASTM UNS ISO Numerical Grade W-Nr. L-Nr. EN Australian Standard AS
7075 7075 A97075 AlZn5.5MgCu A97075 AlZnMgCu1.5 3.4365
A97075
EN-AW-AlZn5.5MgCu 7075
A97075

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!