Grade 04Cr19Ni9Cu2
Other Names
Corresponding Standard Q/YT 102-2019
Stainless Steel Wire Rods for Cold Heading
Classification Austenitic Stainless Steel
04Cr19Ni9Cu2 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu
Minimum Value - - - - - 18 8 2
Maximum Value 0.05 1 2 0.045 0.01 19 10.5 3
04Cr19Ni9Cu2 Mechanical Properties
diameter
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
4.5≤d≤10 Post-Rolling Pickled Condition 530~630 ≥45 ≥65
4.5≤d≤10 Solution Pickled Condition 480~580 ≥50 ≥70
10<d≤16 Post-Rolling Pickled Condition 510~610 ≥45 ≥65
10<d≤16 Solution Pickled Condition 470~560 ≥50 ≥70

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!