Grade GS-13MnNi6-4
Germany W-Nr. 1.6221
Corresponding Standard DIN 17182-1992
General Purpose Steel Castings with Enhanced Weldability and Higher Toughness - Technical Delivery Condition
Classification Cast Steel
GS-13MnNi6-4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N V Nb
Minimum Value 0.08 - 1 - - - 0.8 - - - -
Maximum Value 0.15 0.6 1.7 0.02 0.01 0.3 1.2 0.2 0.02 0.1 0.05
GS-13MnNi6-4 Mechanical Properties
wall thickness
t
mm
Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤500 GS-13MnNi6-4VⅠ Quenching + Tempering (VⅠ) 460~610② ≥300②③ ≥22(A5) Room Temperature: ≥80④
-40°C: ≥27
t≤200 GS-13MnNi6-4VⅡ Quenching + Tempering (VⅡ) 480~630② ≥340②③ ≥20(A5) Room temperature: ≥80④
-40°C: ≥27

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!