Grade C67S
European Standard Steel Grade 1.1231
Corresponding Standard EN 10132-2021
Cold rolled narrow steel strip for heat treatment - Technical delivery conditions
Classification Spring Steel
C67S Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.65 0.15 0.6 - - - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.73 0.35 0.9 0.025 0.025 0.4 0.4 0.3 0.1
① Elements not quoted in this table shall not be intentionally added to the steel without the agreement of the purchaser, other than for the purpose of finishing the heat. All reasonable precautions shall be taken to prevent the addition, from scrap or other material used in manufacture, of such elements which affect the hardenability, mechanical properties and application.
C67S Mechanical Properties
Delivery condition* Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
annealed (+A) or annealed and skin passed(+LC) ≤640 ≤510 ≥16 HV
≤200
cold rolled(+CR)** ≤1140 HV
≤315
quenched and tempered(QT)*** 1200~1900 HV
370~580
• The elongation values in the table are for a gauge length of 80 mm.
• +A=annealed,+LC=annealed and skin passed,+CR=cold rolled,+QT=quenched and tempered
Approximate Comparison Table Spring Steel
Germany France European Standard United Kingdom
DIN EN/DIN NF EN/NF EN Numerical Grade BS EN/BS
Ck67 C68RR C67S 1.1231 CS70
C67S Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!