C75S Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.7 0.15 0.6 - - - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.8 0.35 0.9 0.025 0.025 0.4 0.4 0.3 0.1
① Elements not quoted in this table shall not be intentionally added to the steel without the agreement of the purchaser, other than for the purpose of finishing the heat. All reasonable precautions shall be taken to prevent the addition, from scrap or other material used in manufacture, of such elements which affect the hardenability, mechanical properties and application.
C75S Mechanical Properties
Delivery condition* Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
annealed (+A) or annealed and skin passed(+LC) ≤640 ≤510 ≥15 HV
≤200
cold rolled(+CR)** ≤1170 HV
≤320
quenched and tempered(QT)*** 1200~1900 HV
370~580
• The elongation values in the table are for a gauge length of 80 mm.
• +A=annealed,+LC=annealed and skin passed,+CR=cold rolled,+QT=quenched and tempered
Approximate Comparison Table Spring Steel
United States Germany France European Standard Russia Sweden United Kingdom
AISI UNS DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade GOST SS14 BS EN/BS
1078 G10780 Ck75 1.1248 C75RR C75S 1.1248 75A 1774 CS80
C75S Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!