Grade GX2CrNiMoN25-7-3
European Standard Steel Grade 1.4417
Corresponding Standard EN 10213-2007(+A1:2016)
Steel Castings for Pressure Purposes
Classification Cast Steel
GX2CrNiMoN25-7-3 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo N W
Minimum Value - - - - - 24 6 - 3 0.15 -
Maximum Value 0.03 1 1.5 0.03 0.02 26 8.5 1 4 0.25 1
GX2CrNiMoN25-7-3 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t ≤ 150 Solution Heat Treatment + Water Quenching (AT)① 650~850 ≥480 A: ≥22 Room temperature: ≥50
-70°C: ≥35
GX2CrNiMoN25-7-3 Corresponding Standards(Same grade name, different standards)