Grade 230M07
Corresponding Standard BS 970-3-1991
Specification for wrought steel for machanical and allied engineering purposes part 3:bright bars for general engineering purposes
Classification Carbon Steel
Properties Machinability
230M07 Chemical Element Composition Content (%)
Component C Si Mn P S
Minimum Value - - 0.9 - 0.25
Maximum Value 0.15 0.05 1.3 0.09 0.35
• For older grades of stainless steel, see Table 2 of standard BS 970-4-1970
230M07 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
6≤d<100 Hot rolling + turning or grinding ≥360 ≥215 ≥22 ≥103 -
6≤d≤13 Hot Rolling + Cold Drawing or Hot Rolling + Cold Drawing + Grinding ≥480 ≥400 ≥6 - -
13<d≤16 Hot Rolling + Cold Drawing or Hot Rolling + Cold Drawing + Grinding ≥460 ≥380 ≥7 - -
16<d≤40 Hot Rolling + Cold Drawing or Hot Rolling + Cold Drawing + Grinding ≥430 ≥340 ≥8 - -
40<d≤63 Hot Rolling + Cold Drawing or Hot Rolling + Cold Drawing + Grinding ≥390 ≥280 ≥9 - -
63<d≤76 Hot Rolling + Cold Drawing or Hot Rolling + Cold Drawing + Grinding ≥370 ≥240 ≥10 - -
Approximate Comparison Table Free-Cutting Structural Steel
Taiwan, China Japan South Korea United States Germany France Sweden United Kingdom
CNS JIS KS ASTM/AISI UNS DIN EN/DIN W-Nr. NF EN/NF SS14 BS EN/BS
SUM22 SUM22 SUM22 1213 G12130 9SMn28 1.0715 S250 1912 230M07
230M07 Corresponding Standards(Same grade name, different standards)