Grade GH4133B
Corresponding Standard GB /T 40313-2021
Specification for Wrought Superalloy Forging Disks
Classification Special Alloy Steel
GH4133B Chemical Element Composition Content (%)
Component Fe C Si Mn P S Cr Cu As Ti Nb Zr B Pb Al Sn Mg Ce Bi Sb More
Minimum Value - - - - - - 19 - - 2.65 1.3 0.01 - - 0.75 - 0.001 - - - Ni:余量
Maximum Value 1.5 0.06 0.65 0.35 0.015 0.007 22 0.07 0.0025 3 1.7 0.05 0.01 0.001 1.15 0.0012 0.01 0.01 0.0001 0.0025
GH4133B Mechanical Properties
form Test Temperature Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
sample Room Temperature ≥1060 ≥735 ≥16 ≥18 262~352 KU2
≥31
sample ≥870 Measured ≥15 ≥20 - -
sample High temperature long-term performance:
Stress 392MPa,
Creep fracture time tu ≥ 50h
Stress 343MPa,
Creep fracture time tu ≥ 70h
sample High temperature long-term performance:
Stress 635MPa,
Creep fracture time tu ≥ 100h
GH4133B Corresponding Standards(Same grade name, different standards)