Grade 40CrNi
Corresponding Standard GJB 1220A-2008
Speification for alloy structure steel bar for artillery parts
Classification Alloy Steel
40CrNi Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu
Minimum Value 0.37 0.17 0.5 - - 0.45 1 -
Maximum Value 0.44 0.37 0.8 0.03 0.03 0.75 1.4 0.25
40CrNi Mechanical Properties
diameter
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
d=25 820°C quenching, oil cooling, 500°C tempering, water or oil cooling ≥980 ≥785 ≥10 ≥45 - KU2
≥55
Steel Annealing or Tempering - - - - ≤241 -
40CrNi Corresponding Standards(Same grade name, different standards)