Grade 12CrNi3A
Corresponding Standard GJB 1220A-2008
Speification for alloy structure steel bar for artillery parts
Classification Alloy Steel
12CrNi3A Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu
Minimum Value 0.11 0.17 0.3 - - 0.6 2.75 -
Maximum Value 0.17 0.37 0.6 0.025 0.025 0.9 3.15 0.25
12CrNi3A Mechanical Properties
diameter
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
d=15 860°C First Quenching, 780°C Second Quenching, Water Cooling, 200°C Tempering, Water or Air Cooling ≥930 ≥685 ≥11 ≥50 - KU2
≥71
Steel Annealing or Tempering - - - - ≤217 -