Grade 40CrNiMoA
Corresponding Standard GJB 1220A-2008
Speification for alloy structure steel bar for artillery parts
Classification Alloy Steel
40CrNiMoA Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo
Minimum Value 0.37 0.17 0.5 - - 0.6 1.25 - 0.15
Maximum Value 0.44 0.37 0.8 0.025 0.025 0.9 1.65 0.25 0.25
40CrNiMoA Mechanical Properties
diameter
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
d=25 850°C Quenching, Oil Quenching, 600°C Tempering, Water or Oil Quenching ≥980 ≥835 ≥12 ≥55 - KU2
≥78
Steel Annealing or Tempering - - - - ≤269 -
40CrNiMoA Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!