Grade 35CrNi2Mo
PCrNi2Mo
Corresponding Standard GJB 1220A-2008
Speification for alloy structure steel bar for artillery parts
Classification Alloy Steel
35CrNi2Mo Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo
Minimum Value 0.32 0.17 0.25 - - 0.8 1.75 - 0.2
Maximum Value 0.42 0.37 0.5 0.03 0.03 1.2 2.25 0.25 0.3
35CrNi2Mo Mechanical Properties
diameter
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
d=25 850°C Quenching, Oil Cooling, 600°C Tempering, Oil Cooling ≥930 ≥835 ≥12 ≥50 - KU2
≥78
Steel Annealing or Tempering - - - - ≤255 -